Skip to main content

Table 4 The experimental results of aluminum composite A413 reinforced by 5% Al2O3 powder in two cases of with and without powder in dielectric

From: The effect of alumina powder in dielectric on electrical discharge machining parameters of aluminum composite A413-Al2O3 by the Taguchi method, the signal-to-noise analysis and the total normalized quality loss

Experiment number

Kerosene dielectric (the first test)

Kerosene dielectric containing 3 g/L alumina powder (the second test)

MRR

SR

TWR

MRR

SR

TWR

1

1.223

4.892

0.0311

1.053

4.195

0.0215

2

1.987

9.165

0.0338

1.814

8.443

0.0231

3

2.438

11.938

0.0260

2.269

10.977

0.0162

4

0.814

4.346

0.0341

0.847

3.531

0.0256

5

4.933

8.807

0.0246

3.841

8.231

0.0184

6

2.488

8.337

0.0374

3.015

7.846

0.0329

7

1.578

4.487

0.0238

1.423

3.734

0.0132

8

0.777

9.026

0.0326

0.657

8.924

0.0239

9

4.791

12.941

0.0349

4.599

11.752

0.0258