Table 3 The experimental LCCs for multi-cracked specimens with vertical cracks alignment (Fig. 2b)

From: Ductile failure analysis of epoxy resin plates containing multiple circular arc cracks by means of the equivalent material concept

2β(deg.)

P1 (N)

P2 (N)

P3 (N)

Pavg (N)

  

2a/d = 0.9

  

40

1773

1701

1823

1766

80

1826

1902

1971

1898

120

1962

2176

2080

2072

160

2252

2309

2412

2324

  

2a/d = 0.6

  

40

1707

1859

1912

1828

80

1934

2004

1962

1934

120

2132

2180

2261

2191

160

2289

2453

2395